All of my work is fired to cone 10
reduction in a gas kiln -- a 16 cu. ft. updraft by West Coast Kiln. I
use both stoneware and porcelain cone 10 clays. Testing glazes and learning how to fire my gas kiln
seems to be a lifelong process. I still learn with each firing, and
have had my kiln for 4 years now... Following is a list of glazes I’m
enjoying — culled from Ceramics
Monthly, Clayart, and workshops
I’ve taken:
|
DD Green c10R
gloss
4.98 Barium Carb
4.97 Dolomite 4.97
Gerstley Borate
49.75 Custer Feldspar
24.88 Flint
7.96 Whiting
~97.50 total
…Also add:
2.00 Red Iron Oxide
0.50 Cobalt Carb
0.50 Chrome Oxide
2.00 Bentonite
Shaner's Red
c10 R matt
45.70 Custer Feldspar
3.70 Talc
21.50 EPK
3.50 Bone Ash
18.70 Whiting
5.40 Red Iron Oxide
1.90 Bentonite
Leach White c10
R glossy
40.00 Custer Feldspar
30.00 Flint
20.00 Whiting
10.00 EPK
100.00 total
Also add:
2.00 Tin Oxide
8.00 Zircopax
2.00 Bentonite
Sun Valley
Rutile c10 R glossy
Talc 11.2
Whiting 20.5
Custer 32.2
EPK 16.6
Flint 19.5
Add
Rutile 8.3
Bentonite 2 |
Coleman Purple c10 R glossy
4.98 Barium Carb
4.97 Dolomite
4.97 Gerstley Borate
2.49 Zinc Oxide
49.75 Custer Feldspar
24.88 Flint
7.96 Whiting
100.00 total
Also add:
1.00 Tin Oxide
0.25 Cobalt Carb
2.00 Copper Carb
Steven Hill's Fake Blue Ash c10
F-4 6.82%
Dolomite 3.79%
Whiting 45.45%
EPK 30.30%
Flint 13.64%
total… 100.00%
Bentonite 2.27%
Red Iron Oxide 1.00%
Cobalt Carbonate
1.14%
Penland Mamo c10 R matt
Custer Feldspar
53.26%
EPK 21.74%
Whiting 4.35%
Dolomite 20.65%
total… 100.00%
Tin Oxide 2.00%
Zircopax 8.00%
Bentonite 2.00%
Waxy Turquoise c10 R satin matt
Flint 19.8
Custer 40.59
EPK 4.95
Talc 14.85
Gerstley Borate 11.88
Dolomite 6.93
Chrome Oxide 0.5
Cobalt Ox 0.5 |
|
|
|
|
|
|
|
|
|
|
Coleman-Purple, Waxy Turquoise bowl |
|
|
|
|
|
|
|
|
|
|
|
|
Nesting Bowls, Stoneware triple-dip |
|
|
|
|
|
|
|
|
|
|
|
|
Copper Red and Coleman Teal Tea Set |
|
|
|
|
|
|
|
|